Physical Properties |
Metric |
English |
Comments |
Density |
1.65 g/cc |
0.0596 lb/in³ |
Water Absorption |
0.0200 % |
0.0200 % |
Linear Mold Shrinkage, Flow |
0.00200 - 0.00600 cm/cm |
0.00200 - 0.00600 in/in |
Linear Mold Shrinkage, Transverse |
0.00400 - 0.00600 cm/cm |
0.00400 - 0.00600 in/in |
|
Mechanical Properties |
Metric |
English |
Comments |
Hardness, Rockwell M |
100 |
100 |
Tensile Strength at Break |
150 MPa |
21800 psi |
Elongation at Break |
1.20 % |
1.20 % |
Tensile Modulus |
15.7 GPa |
2280 ksi |
Flexural Modulus |
15.0 GPa |
2180 ksi |
Flexural Strength |
230 MPa |
33400 psi |
Charpy Impact Unnotched |
2.80 J/cm² @Temperature 23.0 °C |
13.3 ft-lb/in² @Temperature 73.4 °F |
|
2.80 J/cm² @Temperature -30.0 °C |
13.3 ft-lb/in² @Temperature -22.0 °F |
Charpy Impact, Notched |
0.700 J/cm² @Temperature 23.0 °C |
3.33 ft-lb/in² @Temperature 73.4 °F |
|
0.700 J/cm² @Temperature -30.0 °C |
3.33 ft-lb/in² @Temperature -22.0 °F |
Izod Impact, Notched (ISO) |
7.00 kJ/m² @Temperature -30.0 °C |
3.33 ft-lb/in² @Temperature -22.0 °F |
|
7.00 kJ/m² @Temperature 23.0 °C |
3.33 ft-lb/in² @Temperature 73.4 °F |
|
Electrical Properties |
Metric |
English |
Comments |
Volume Resistivity |
>= 1.00e+13 ohm-cm |
>= 1.00e+13 ohm-cm |
Surface Resistance |
>= 1.00e+15 ohm |
>= 1.00e+15 ohm |
Dielectric Constant |
4.70 @Frequency 1.00e+6 Hz |
4.70 @Frequency 1.00e+6 Hz |
|
4.70 @Frequency 10000 Hz |
4.70 @Frequency 10000 Hz |
Dielectric Strength |
25.0 kV/mm |
635 kV/in |
Dissipation Factor |
0.00800 @Frequency 10000 Hz |
0.00800 @Frequency 10000 Hz |
|
0.0200 @Frequency 1.00e+6 Hz |
0.0200 @Frequency 1.00e+6 Hz |
|
Thermal Properties |
Metric |
English |
Comments |
CTE, linear, Parallel to Flow |
0.200 µm/m-°C |
0.111 µin/in-°F |
CTE, linear, Transverse to Flow |
0.410 µm/m-°C |
0.228 µin/in-°F |
Melting Point |
280 °C |
536 °F |
Deflection Temperature at 0.46 MPa (66 psi) |
215 °C |
419 °F |
Deflection Temperature at 1.8 MPa (264 psi) |
270 °C |
518 °F |
Glass Transition Temp, Tg |
90.0 °C |
194 °F |
Flammability, UL94 |
V-0 @Thickness 1.50 mm |
V-0 @Thickness 0.0591 in |
|
V-0 @Thickness 0.850 mm |
V-0 @Thickness 0.0335 in |
Oxygen Index |
47.0 % |
47.0 % |
|
Processing Properties |
Metric |
English |
Comments |
Feed Temperature |
60.0 - 80.0 °C |
140 - 176 °F |
Nozzle Temperature |
310 - 330 °C |
590 - 626 °F |
Zone 1 |
290 - 300 °C |
554 - 572 °F |
Zone 2 |
310 - 320 °C |
590 - 608 °F |
Zone 3 |
330 - 340 °C |
626 - 644 °F |
Zone 4 |
330 - 340 °C |
626 - 644 °F |
Melt Temperature |
310 - 340 °C |
590 - 644 °F |
|
330 - 340 °C |
626 - 644 °F |
Mold Temperature |
135 - 160 °C |
275 - 320 °F |
|
140 - 160 °C |
284 - 320 °F |
Drying Temperature |
130 - 140 °C |
266 - 284 °F |
Dry Time |
3 - 4 hour |
3 - 4 hour |
Moisture Content |
<= 0.0200 % |
<= 0.0200 % |
Injection Pressure |
50.0 - 100 MPa |
7250 - 14500 psi |
Hold Pressure |
30.0 - 70.0 MPa |
4350 - 10200 psi |
Back Pressure |
0.000 - 3.00 MPa |
0.000 - 435 psi |
Screw Speed |
50.0 rpm @Diameter 55.0 mm |
50.0 rpm @Diameter 2.17 in |
|
75.0 rpm @Diameter 40.0 mm |
75.0 rpm @Diameter 1.57 in |
|
120 rpm @Diameter 25.0 mm |
120 rpm @Diameter 0.984 in |
|
Descriptive Properties |
Hopper |
20-30°C |
Manifold |
330-340°C |